Titanium Anode Manufacturing

Looking for a titanium anode manufacturer that controls the whole process in house? This guide covers our DSA anode production line step by step, explains how we match Ru-Ir, Ir-Ta, platinized, and PbO₂ coatings to each application, and shares what 20 years of coating experience means for your electrode life.

Table of Contents

DSA Coated Titanium Anode

hree systems keep a vessel’s underwater structure fit for service. An ICCP system stops hull corrosion by impressing protective current through MMO or platinized titanium anodes. A marine growth prevention system (MGPS) keeps seawater cooling lines clear by dosing copper and aluminum ions. A shaft grounding device bleeds stray current off the propeller shaft before it destroys bearings. This guide explains how each system works, the design numbers that matter, and the maintenance intervals that keep them reliable.

Key design values at a glance

ParameterDesign value
Hull protection potential (vs. Ag/AgCl reference)-0.85 to -1.10 V
ICCP auxiliary anode materialsMMO coated titanium or platinized titanium (Pt layer 5 µm or thicker)
Reference electrode accuracy / life±10 mV / 5 years or longer
Effective copper ion level for MGPS dosingAbout 2 mg/m³ in seawater
Shaft-to-hull potential difference target50 mV or lower (30 mV design target, ISO 19036:2016)
Shaft grounding circuit resistance0.01 Ω or lower

Why One Protection System Is Never Enough

Seawater attacks a ship in three distinct ways. It corrodes the hull and underwater structure electrochemically. It carries marine organisms that colonize sea chests, condensers, and cooling piping. And the electrical plant itself drives stray currents through the shaft line. Each failure mode needs its own countermeasure, so shipbuilders fit three: an impressed current cathodic protection (ICCP) system for the hull, a marine growth prevention system  for the seawater side, and a shaft grounding device for the propeller shaft. Together they form the protective barrier around the underwater part of the ship.

ICCP: Active Corrosion Protection for the Hull

Sacrificial anodes versus impressed current

Cathodic protection comes in two forms. The sacrificial anode method connects a more active metal, typically zinc or aluminum, directly to the steel structure. The anode dissolves and supplies protective current to the steel. Ships using this method fit zinc anode blocks along the bilge keel flowline, in sea chests, inside double bottoms and void spaces, and on the rudder and propeller. Aluminum alloy anodes perform better than zinc, but classification rules prohibit them in machinery spaces and cargo oil tanks because their high operating potential can generate sparks. Sacrificial anodes carry a design life of 2 to 3 years and are inspected and renewed as a set at every drydocking.

An ICCP system takes the opposite approach. Instead of consuming metal, it uses external power and long-life anodes to drive protective current, which makes it the active defense layer for the hull.

How ICCP works

Steel immersed in seawater corrodes through anodic oxidation: Fe → Fe²⁺ + 2e⁻. The metal literally dissolves as it loses electrons. An ICCP system counters this by pushing the hull potential negative into the protected range. Hold the steel below -0.85 V against a silver/silver chloride reference electrode (measured in 3.5% sodium chloride solution at 25°C) and the dissolution rate falls below roughly 0.01 mm per year, low enough to ignore over a docking cycle.

The system holds that potential with a closed control loop. Reference electrodes on the hull feed potential readings to the potentiostat, which uses PID control with about ±1% regulation accuracy to trim its output current. If the potential drifts above roughly -0.8 V the hull is under-protected and the system raises the current. If it falls below about -1.1 V the hull is over-protected, which risks paint disbondment and hydrogen embrittlement of the steel, so the system cuts the current back immediately.

Seawater conditions shift the targets. For every 10°C rise in water temperature the protection potential needs to move about 50 mV more negative. When salinity drops by 10 parts per thousand, for example entering an estuary, conductivity falls with it, so current density should be reduced by around 15% to avoid wasting energy.

The four building blocks

ComponentFunctionTypical specification
Potentiostat (transformer-rectifier)The control brain. Regulates output current from reference electrode feedback.Output range 0 to 500 A depending on wetted hull area; holds potential between -0.85 and -1.10 V
Auxiliary anodeDischarges protection current into the seawater.Platinized titanium (Pt layer 5 µm or thicker) or MMO coated titanium; polarization overpotential 0.3 V or lower at 100 A/m²
Reference electrodeMeasures actual hull potential.Solid-state Ag/AgCl, accuracy ±10 mV, service life 5 years or longer; mounted at least 2 m from any anode
Monitoring networkVerifies protection is uniform over the whole hull.5 to 8 reference electrodes spaced no more than 15 m apart; voltmeter input impedance 100 MΩ or higher, 0.01 V resolution

Installation note: the blasted and painted area around each anode must meet coating thickness and quality requirements, otherwise current shorts through the coating and protection fails locally.

Why MMO coated titanium leads for auxiliary anodes

The auxiliary anode is the component that decides service life. Platinized titanium anodes should consume no more than about 1 g per ampere-year, and the anode is due for replacement once the platinum layer wears below 2 µm. MMO coated titanium anodes deliver comparable or better durability at high current density in seawater, with a mixed metal oxide layer fired onto a titanium substrate that resists the demanding polarity conditions of ICCP service. For anode selection, confirm the coating is qualified for continuous seawater duty at the specified current density, and check the mounting insulation before commissioning.

Two lessons from fleet service

 On one 100,000 DWT tanker in the Indian Ocean, the ICCP anode current jumped suddenly from 80 A to 250 A while the protection potential held steady at -0.9 V. The crew suspected an anode short, but a short would have pulled the anode potential sharply down. The real cause was a grounding incident that stripped about 20 m² of bottom paint. Bare steel demands roughly 120 mA/m² of protection current, against 10 to 20 mA/m² for painted areas, so the system correctly raised its output to hold potential. Caught late, a bare patch like that can show visible rust within a month.

Over-protection is real damage, not a safety margin.

 On a container ship, a failed potentiostat let the protection potential drift down to -1.2 V. Three months later the docking survey found bottom paint blistered and detached over large areas, with hydrogen cracking in the exposed plate.

ICCP maintenance essentials

  • Check panel readings every watch. Record potential and current values daily. Expect current swings alongside berthing and canal transits in confined waters; these are normal.
  • Calibrate reference electrodes against standard solution once per voyage. Replace any electrode that drifts more than 20 mV.
  • Measure anode insulation resistance every six months. It should stay above 10 MΩ.
  • Track anode consumption. Replace platinized anodes once the platinum layer falls below 2 µm.
  • At docking, inspect anode surfaces for scale. Clean with high-pressure fresh water only. Never scrape the coating with hard tools.
  • If potential drifts positive beyond -0.8 V, check first for reference electrode fouling or damaged cable insulation. If current spikes while potential stays stable, look for hull coating damage or an anode short.

MGPS: Keeping Seawater Cooling Lines Clear

The fouling problem

Marine organisms that settle inside sea chests and cooling piping restrict flow, raise cooling water temperatures, and force main engine load reductions. Once established, colonies are expensive to remove. The MGPS prevents settlement rather than fighting established growth, which is why every seawater-cooled system benefits from one.

How an MGPS works

There are two working principles in common service.

Anode dosing systems electrolyze copper, aluminum, or iron anodes mounted in the seawater stream. The current loop runs between the anodes and the hull, not between the anodes themselves. Copper anodes release trace copper ions, effective at levels around 2 mg/m³, that poison barnacle and mussel larvae before they can settle. Aluminum anodes release aluminum hydroxide floc that traps larvae mechanically, and the same floc lays down a thin film on pipe walls that adds a barrier against seawater corrosion. The anode grade matches the piping material: steel piping takes copper and aluminum anodes, while aluminum or copper piping takes iron anodes. Consumable anodes last 2 to 3 years and are renewed at docking.

Direct seawater electrolysis systems use a titanium plate, insulated from the hull, as the anode with the hull itself as the cathode. Electrolysis of the seawater generates oxidants in situ, the same chemistry behind electrochlorination, and no consumable metal is shipped or dosed.

Anode dosing systems face growing environmental scrutiny because they discharge copper and aluminum directly to sea, and both are non-renewable consumables. Several developed countries now discourage their use, which is why direct electrolysis designs are gaining ground in newbuilds.

 

Send us an Inquirty